Cause analysis of defects in valve casting during production

Time:2018-11-24
1. The stomataThis is a small cavity formed by the gas that cannot be escaped from the metal during solidification. Its inner wall is smooth and contains gas, and it has a high reflectivity to ultrasonic wave.

1. The stomata

This is a small cavity formed by the gas that cannot be escaped from the metal during solidification. Its inner wall is smooth and contains gas, and it has a high reflectivity to ultrasonic wave. However, because it is basically spherical or ellipsoidal, it is also a point defect, which affects its reflected amplitude. After forging or rolling, the pores in ingots are compressed into area defects, which are favorable for ultrasonic detection.

2. Shrinkage cavity and porosity

When the casting or ingot is cooled and solidified, the volume should shrink, and the final solidified part can not be replaced by liquid metal, thus forming a void defect. Large and concentrated voids are called shrinkage holes, and small and dispersed voids are called loose. They are generally located in the last solidified part of the ingot or casting center. The inner wall is rough, and there are many impurities and small pores around them. Due to the law of thermal expansion and cold shrinkage, shrinkage holes are inevitable, but they have different shapes, sizes and positions with different processing methods. When they extend to casting or ingot body, they become defects. If the shrinkage cavity is not removed and brought into the forgings, the ingot will become the residual shrinkage cavity (shrinkage cavity residual, residual shrinkage pipe).

3. The slag

Slag inclusion defect is formed when the slag or refractory material on the furnace body breaks off and enters the liquid metal during the melting process and gets involved in the casting or ingot body during pouring. Slag inclusion usually does not exist in a single, often dense state or dispersed in different depths, it is similar to the volume type of defects but often have a certain degree of linearity.

4. The inclusions

Reaction products (such as oxides, sulphides, etc.) in the melting process - non-metallic inclusion, or some components of the metal components of the additive material is not completely melted and residual metal inclusion, such as high density, high melting point components - tungsten, molybdenum, etc.

5. Segregation

The segregation of castings or ingots mainly refers to the composition segregation caused by uneven distribution of components in the smelting process or the melting process of metals. The mechanical properties of regions with segregation are different from the mechanical properties of the entire metal matrix, and the difference beyond the allowable standard range becomes a defect.

6. Casting cracks

Of casting cracks is mainly due to the metal cooling solidification contraction caused by the stress exceeds the limit of material strength, it is related to the shape of the casting design and casting process, also with some high content of impurities in the metal materials caused by cracking sensitivity about (such as sulfur content high brittleness, high phosphorus content with cold brittleness, etc.). Axial crystal cracks may also occur in ingots. If they cannot be forged together in the subsequent open-billet forging, they will remain in the forgings and become internal cracks in the forgings.

7. Cold insulation

This is a kind of stratification peculiar to the casting defects, mainly related to the casting casting process design, when it is pouring liquid metal, due to interruption of splash, double wave, pouring, or from two different directions (or more) metal flow meet, because the liquid metal semi-solid film on the casting cooling formation on the surface of the body and form a membrane of the area of defects.

8. Skull patch

This is when the steel from ladle to mold casting ingot, because pouring interrupt, pause, first poured into the surface of the liquid metal rapidly cooled in air oxidation film formation, continuing pouring new pouring into the liquid metal to break through its turn into steel ingot and formed a kind of stratification (area) defect, it is not in the subsequent breakdown of ingot forging forging close to eliminate.

anisotropy

When casting or steel ingot is cooled and solidified, the cooling speed from the surface to the center is different, so different crystal structures will be formed, which is manifested as anisotropy of mechanical properties, and also leads to anisotropy of acoustic properties, that is, there are different sound velocities and sound attenuation from the center to the surface. The existence of this anisotropy will have a bad effect on the size and position of casting defects in ultrasonic testing.

主站蜘蛛池模板: 免费观看一级欧美片 | 91精品视频在线播放 | 黄色a级一级片 | 美女视频黄的免费的 | 91在现视频 | 国产精品国产三级国产专区50 | 99精品视频在线看 | 99久久精品免费 | 日本黄色一级 | 亚洲精品久久7777777 | 久热这里只有 | 国产一区二区三区伦理 | 免费a级毛片在线播放 | 日本精品在线播放 | 精品视频在线观看免费 | a软片免费看在线 | a级一级片 | 99re视频在线免费观看 | 99国产在线观看 | 国产乱淫av免费 | 久久毛片高清国产 | 麻豆国产一区二区三区 | 一级一片免费看 | 91麻豆精品久久久久蜜臀 | 伊人婷婷涩六月丁香七月 | 国产亚洲欧美在线 | 欧美国产精品日韩约炮 | 日日操夜夜操免费视频 | 国产精品麻豆99久久久久久 | av不卡一区二区 | 欧美激情视频网站 | 韩国黄色录像一级片 | 国产免费观看网站 | 国产大片免费完整观看 | 精品一二三区视频 | 亚州国产精品 | 91丨九色丨国产 | 成人免费视频中文字幕 | 一区二区视频网 | 91欧美在线视频 | 欧美特黄特色视频 |